Title of Invention

METHOD FOR PRODUCTION OF A THIN-LAYER SOLAR CELL WITH MICROCRYSTALLINE SILICON AND LAYER SEQUENCE

Abstract The invention relates to a method for production of a thin-layer solar cell with microcrystalline silicon and a-layer sequence. According to the invention, a microcrystalline silicon layer is applied to the lower p- or n-layer in pin or nip thin-layer solar cells, by means of a HWCVD method before the application of the microcrystalline i-layer. The efficiency of the solar cell is hence increased by up to 0.8 % absolute.
Full Text 23957 PCT/DE2005/002237 Transl. of WO 2006/066544
METHOD FOR PRODUCING A THIN-FILM SOLAR CELL BY USE OF
MICROCRYSTALLINE SILICON AND A LAYER SEQUENCE
The invention relates to a method for producing a thin-
film solar cell by use of microcrystalline silicon and a layer
sequence.
Microcrystalline thin-film solar cells comprise various
layers of silicon that differ in their doping and degree of
crystallinity. The layers are deposited on substrates such as
glass. Various methods are known for this purpose. In the PECVD
method a gas mixture is decomposed into fragments in a plasma, and
in the HWCVD method the gas or gas mixture is decomposed by heating
a wire. In both methods decomposition products deposit on the
substrate, resulting in a coating. The photo-CVD method and
sputtering, known from the prior art, may also be used to deposit
layers on surfaces.
A distinction is made between pin cells and nip cells,
that differ in their layer sequence.
In a pin solar cell the layer adjoining the transparent
substrate is a p-layer, i.e. :a p-doped silicon layer; the i-layer
is located on the p-layer and is not doped. The n-layer, that is
n-doped, is located on the i-layer. In a nip solar cell the p-
layer and the n-layer are exchanged with one another, and likewise
include an i-layer.
The microcrystalline p-layer is p-doped silicon that is
doped with boron, for example.
One skilled in the art is familiar with the manner in
which these layers are deposited.
- 1 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
For a p-layer, gas mixtures containing silicon compounds,
positively doped compounds such as boron compounds, as well as
hydrogen gas are used that are decomposed and deposited on the
surface. The resulting layer is microcrystalline. The known
HWCVD, PECVD, and photo-CVD methods may be used for this purpose.
For the deposition of the microcrystalline i-layer, a
mixture comprising a silicon compound and hydrogen is decomposed,
whereupon a microcrystalline Si layer is deposited. The known
HWCVD, PECVD, sputtering, and photo-CVD methods may likewise be
used for this purpose.
For the deposition of the microcrystalline n-layer, a
mixture comprising a silicon-containing compound, hydrogen, and
negatively doped compounds such as phosphorus-containing compounds
is decomposed. The HWCVD, PECVD, and photo-CVD methods may be used
here as well.
According to one known method, thin-film solar cells are
deposited onto transparent substrates by means of PECVD. The
deposition sequence is pin or also nip, the individual layers
generally being deposited in different cavities. For PECVD the
microcrystalline layers are deposited by use of various possible
excitation frequencies, such as radio frequencies, microwave, or
very high frequency (VHF). High plasma outputs are necessary for
achieving high deposition rates by means of PECVD. The HWCVD
method requires high wire temperatures for achieving high
deposition rates. Solar cells having a low fill factor and a low
open circuit voltage have heretofore been produced at high
deposition rates. The HWCVD method is also much more time-
intensive than the PECVD method. Solar cells having very high Voc
and FF may be obtained at low substrate temperatures.
- 2 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
The object of the invention is to provide a method for
producing solar cells that results in solar cells having higher
efficiency, in particular higher Voc and FF. An aim is to increase
the open circuit voltage of the solar cells by use of the method.
A further aim is to provide a layer sequence having characteristics
that allow higher open circuit voltages and fill factors. It
should be possible to carry out the method in the shortest possible
time.
Proceeding from the preamble of claim 1, the object
according to the invention is achieved by the features stated in
the characterizing clause of claim 1.
The method according to the invention may be used to
produce pin and nip solar cells based on microcrystalline silicon
that have a higher efficiency, i.e. a higher open circuit voltage
(Voc) and a higher fill factor (FF).
Advantageous refinements of the invention are described
in the subclaims.
The invention is explained below.
For the production of the solar cells or layer sequences
according to the invention, in a first step a transparent current-
conducting layer is deposited on a transparent substrate, for
example glass or plastic, which is referred to in the technical
field as a TCO layer. This layer typically has a layer thickness
of 0. 5B2 jxm, and may have, but is not limited to, the following
composition: SnO2, ZnO, ITO.
The deposition may be carried out using conventional
methods, for example sputtering or CVD.
The method according to the invention is explained below
for a pin solar cell. However, the invention also encompasses the
- 3 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
production of a nip solar cell. In the production of the latter
the same steps are carried out, except that the sequence of
application of the p-layer and the n-layer is reversed.
In a further step, on the TCO layer a microcrystalline p-
layer is deposited onto the transparent substrate together with the
superposed TCO layer, preferably by use of the PECVD method.
However, the deposition may also be performed using other methods
known from the prior art, such as the HWCVD method, sputtering, or
the photo-CVD method.
This step is carried out using method parameters and gas
mixtures known to one skilled in the art.
Gas mixture components comprise a silicon-containing
compound, hydrogen, and a compound that deposits a substance that
results in p-doping.
The silicon-containing compound may be, but is not
limited to, at least one component from the group comprising SiH4,
methyl silane, dimethyl silane, trimethyl silane, tetramethyl
silane, disilane, trisilane, or halosilanes such as HSiCl3, H2SiCl2,
HsSiCl1, SiCl4, or the corresponding fluorine compounds.
The concentration of the silicon compounds is, for
example, between 0.1% and 10%.
The total pressure may be, for example, between 0.2 hPa
and 2 0 hPa.
The compound that deposits the component that results in
p-doping may be, but is not limited to, at least one component of
the group comprising diborane, trimethylborane, or organyl
compounds of Ga and Al, such as trimethyls or triethyls.
- 4 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
The concentration of the p-doped compound is, for
example, between 0.1% and 2%, relative to the silicon-containing
compound.
The gas mixture, which comprises the silicon-containing
compound, the compound that deposits the component that results in
p-doping, and hydrogen as substitutes is decomposed by means of the
PECVD method or another method such as the HWCVD method or the
photo-CVD method, and the resulting components deposit in the form
of a microcrystalline p-doped silicon layer.
The substrate temperature may, for example, be between
50EC and 300EC.
The depositing layers have a layer thickness of
2 nmBlOO nm, preferably 5 nmB30 nm, particularly preferably
10 nmB20 nm.
In the next step, according to the invention a
microcrystalline silicon layer is deposited by the HWCVD method.
Surprisingly, it has been shown that the deposition of a layer of
microcrystalline silicon by the HWCVD method results in an increase
in the open circuit voltage and the fill factor, and thus the
efficiency of solar cells. The layer thickness of the layer
deposited by means of the HWCVD method may be 2 nmB200 nm,
preferably 5. nmB50 nm, particularly preferably 10 nmB20 nm.
For the deposition of the above-referenced layer, a gas
comprising hydrogen and a silicon-containing compound that may be,
but is not limited to, SiH4, disilane, trisilane, or halosilanes
such as HSiCl3, H2SiCl2, H3SiCl1, SiCl4, or the corresponding
fluorine compounds is used.
- 5 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
For carrying out the method step according to the
invention, the parameters preferably are, but are not limited to,
the following:
Wire material: tungsten, tantalum, graphite, rhenium, or
osmium, or high-melting materials.
Wire temperature: 1200ECB2200EC (or preferably
1500EB1800EC)
Substrate temperature: Pressure: 1 PaBlOO Pa (or preferably 2 PaBlO Pa)
Hydrogen dilution: 0.1%B20% silane in hydrogen.
The layer produced according to these parameters
(produced by HWCVD) has a thickness of 2 nmB200 nm, preferably
5 nmB20 nm, and has a crystallinity of > 0%.
The substrate temperatures are preferably between 50EC
and 300EC, particularly preferably between 150EC and 200EC.
The gas concentrations are, for example, 0.1B10% silane
or silicon-containing compound, relative to hydrogen.
The total pressure range is between 1 Pa and 100 Pa.
This microcrystalline silicon layer applied as an
intermediate layer causes the overall solar cell to have a higher
open circuit voltage and a higher fill factor, and thus a higher
efficiency. This layer forms a part of the microcrystalline i-
layer that is applied to the p-doped layer.
The absolute efficiency is increased by up to 0.8%, the
open circuit voltage by up to 25 mV, and the fill factor by up to
3%.
In a further step, preferably by use of the PECVD method,
an additional microcrystalline silicon i-layer is deposited. In
- 6 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
this method step, the same as for the other steps, alternative
methods such as HWCVD, sputtering, or photo-CVD may be used.
In principle, the deposition may be carried out using the
same components as for the deposition of the intermediate layer.
The compounds used for the deposition are hydrogen and at
least one component from the group comprising, but not limited to,
SiH4, disilane, trisilane, or halosilanes such as HSiCl3, H2SiCl2,
H3SiCl1, SiCl4, or the corresponding fluorine compounds.
This layer preferably has a crystallinity of > 20%.
The silane concentrations or the concentration of the
silicon-containing compound may be, for example, 0.1%B100%.
Hydrogen may optionally be present.
The temperature range is preferably 50B400EC,
particularly preferably 150ECB200EC for pin layer sequences, or
150EB250EC for nip layer sequences.
The total pressure is, for example, between 0.2 hPa and
20 hPa.
The layer thickness of the microcrystalline i-layer
deposited by the PECVD method is preferably between 0.2 μm. and
10 μm, particularly preferably between 0.5 μm and 2 μm.
Characteristics of the i-layer:
Produced by PECVD (RF, VHF, microwave, etc.)
Thickness: preferably 0.5 μmB5 μm
Crystallinity: > 20%.
The layer deposited by use of the HWCVD method and the
PECVD method forms an i-layer of microcrystalline silicon, which
compared to an i-layer according to the prior art allows a higher
- 7 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
open circuit voltage, a higher fill factor, and a higher
efficiency.
An n-layer is deposited on the i-layer.
The n-layer may be amorphous or microcrystalline.
To this end, a gas mixture comprising a silicon-
depositing compound, optionally hydrogen, and a component that
causes n-doping is used.
The component used as the silicon-depositing component
may for example be, but is not limited to, SiH4, methyl silane,
dimethyl silane, trimethyl silane, tetramethyl silane, or HSiCl3,
H2SiCl2, H3SiCli, or SiCl4.
Phosphine, for example, may be used as an n-doping
compound.
The deposition of the n-doped layer may be carried out
using the PECVD method, photo-CVD method, sputtering, or HWCVD
method, for example.
The layer thickness of the n-layer is preferably between
5 nm and 50 nm, particularly preferably between 10 nm and 30 nm.
The preferred coating temperatures are between 100EC and
400EC.
The total pressure is typically between 0.2 hPa and
20 hPa.
The concentration of the silicon-containing compound in
the gas phase is between 0.1% and 100%.
Phosphine is used in a concentration range that is
preferably between 0.1% and 5%, relative to silane or the silicon-
containing compound.
The percentage values in each case refer to volume
percent.
- 8 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
The topmost layer, i.e. for pin the n-layer and for nip
the p-layer, is usually coated with a reflective layer. This
reflective layer may, for example, be composed of a TCO layer and a
metal layer made of Ag or Al, for example.
The invention also encompasses stacks of layers that
contain the layer sequence according to the invention at least
once.
The invention also encompasses layer sequences having the
following patterns:
A) a microcrystalline p-layer,
a microcrystalline intrinsic silicon layer applied
by the HWCVD method,
an i-layer applied by the PECVD method, and
a microcrystalline or amorphous n-layer
or also a thin-film solar cell comprising:
B a transparent substrate,
B a TCO layer,
B a microcrystalline p-layer,
B a microcrystalline intrinsic silicon layer applied
by the HWCVD. method,
B an i-layer applied by the PECVD method,
B a microcrystalline or amorphous n-layer, and
B a reflective layer.
B) a microcrystalline n-layer.
a microcrystalline intrinsic silicon layer applied
by the HWCVD method,
an i-layer applied by the PECVD method, and
a microcrystalline or amorphous p-layer
or also a thin-film solar cell comprising:
- 9 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
B a transparent substrate,
B a TCO layer,
B a microcrystalline n-layer,
B a microcrystalline intrinsic silicon layer applied
by the HWCVD method,
B an i-layer applied by the PECVD method,
B a microcrystalline or amorphous p-layer, and
B a reflective layer.
The p, n, and TCO layers are conventional, and are not
limited to the parameters and production methods illustrated in the
description.
Example:
A 5B50 nm thick intrinsic HW layer was deposited on the
p-layer that had been deposited onto a ZnO substrate by VHF-PECVD.
This layer was deposited at a wire temperature of 1650EC, 3.5 Pa,
and 2B1O% silane in hydrogen, at a deposition rate of 1B2 A/s. The
production of the solar cell was continued with the deposition of
the i-layer by VHF-PECVD at a high growth rate. The open circuit
voltage was thus increased by 20 mV, the fill factor by 2%, and the
absolute efficiency by 0.8%.
The advantageous characteristics of the solar cell
according to the invention are shown in the figures:
FIG. 1 illustrates the comparison of the open circuit
voltages of pin solar cells with and without the intermediate layer
according to the invention.
The silane concentration for the i-layer deposition is
plotted on the abscissa in %.
- 10 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
The ordinate shows the open circuit voltages obtained, in
mV.
The circles represent solar cells without the
intermediate layer according to the invention, and the triangles
represent solar cells with the intermediate layer according to the
invention. It is seen that the open circuit voltage is increased
according to the invention.
FIG. 2 shows the comparison of the fill factors of pin
solar cells with and without the intermediate layer according to
the invention.
The silane concentration for the i-layer deposition is
plotted on the abscissa in %.
The ordinate shows the fill factors obtained, in %.
The circles represent solar cells without the
intermediate layer according to the invention, and the triangles
represent solar cells with the intermediate layer according to the
invention. It is seen that the fill factors are increased
according to the invention.
- 11 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
Claims
1. A method for producing a thin-film solar cell in
which a pin or nip layer sequence is produced,
characterized in that
the following layers are successively deposited:
a) a microcrystalline p- or n-layer
b) a microcrystalline silicon layer that is applied by an
HWCVD method,
c) a microcrystalline i-layer,
d) if a p-layer is present as layer a), an n-layer, and
if an n-layer is present as layer a), a p-layer, which may be
either microcrystalline or amorphous.
2. The method according to claim 1,
characterized in that
layer b) is applied in a layer thickness of 2 nmB200 nm.
3. The method according to claim 2,
characterized in that
layer b) is applied in a layer thickness of 5 nmB50 nm.
4. The method according to one of claims 2 or 3,
characterized in that
layer b) is applied in a layer thickness of 10 nmB20 nm.
5. The method according to one of claims 1 through 4,
characterized in that
- 12 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
for the deposition of layer b) at least one component of
the silicon compounds from the group comprising SiH4, disilane,
trisilane, or halosilanes such as HSiCl3, H2SiCl2, H3SiCli, or SiCl4
is used.
6. The method according to one of claims 1 through 5,
characterized in that
in the HWCVD method a wire composed of materials from the
group comprising tungsten, tantalum, graphite, rhenium, or osmium
is used.
7. The method according to one of claims 1 through 6,
characterized in that
the wire for producing layer b) is heated to a
temperature of 1200EC to 2200EC.
8. The method according to one of claims 1 through 7,
characterized in that
the substrate temperature in the production of layer b)
is 9. The method according to one of claims 1 through 8,
characterized in that
the process pressure in the production of layer b) is 1
PaBlOO Pa.
10. The method according to claim 9,
characterized in that
the process pressure is 2 PaBlO Pa.
- 13 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
11. The method according to one of claims 1 through 10,
characterized in that
the gas concentration of silane or silicon-containing
compound is 0.1%B20% by volume.
12. The method according to one of claims 1 through 11,
characterized in that
the substrate temperature is between 50EC and 300EC.
13. The method according to claim 12,
characterized in that
the substrate temperature is between 150EC and 200EC.
14. A layer sequence comprising the following layers:
B a microcrystalline p-layer,
B a microcrystalline silicon layer applied by the
HWCVD method,
B a microcrystalline i-layer applied by the PECVD
method, and
B a microcrystalline or amorphous n-layer.
15. The layer sequence according to claim 14,
characterized in that
the microcrystalline silicon layer applied by the HWCVD
method is a layer that has been applied according to one of the
method steps of claims 2 through 13.
- 14 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
16. The layer sequence according to one of claims 14 or
15,
characterized in that
the microcrystalline p-layer is situated on a TCO layer
that is applied to a transparent medium.
17. The layer sequence according to one of claims 14
through 16,
characterized in that
a reflective layer or a stack of additional layers is
situated above the n-layer.
18. A layer sequence comprising the following layers:
B a microcrystalline n-layer,
B a microcrystalline silicon layer applied by the
HWCVD method,
B a microcrystalline i-layer applied by the PECVD
method, and
B a microcrystalline or amorphous p-layer.
19. The layer sequence according to claim 18,
characterized in that
the microcrystalline silicon layer applied by the HWCVD
method is a layer that has been applied according to one of the
method steps of claims 2 through 13.
20. The layer sequence according to one of claims 18 or
19,
characterized in that
- 15 -

23957 PCT/DE2005/002237 Transl. of WO 2006/066544
the microcrystalline n-layer is situated on a TCO layer
that is applied to a transparent medium.
21. The layer sequence according to one of claims 18
through 20,
characterized in that
a reflective layer or a stack of additional layers is
situated above the p-layer.
22. A thin-film solar cell comprising a layer sequence
according to one of claims 14 through 21.
23. A thin-film solar cell,
characterized in that
the thin-film solar cell has been produced according to
one of claims 1 through 13.
- 16 -

The invention relates to a method for production of a thin-layer solar cell with microcrystalline silicon and a-layer
sequence. According to the invention, a microcrystalline silicon layer is applied to the lower p- or n-layer in pin or nip thin-layer
solar cells, by means of a HWCVD method before the application of the microcrystalline i-layer. The efficiency of the solar cell is
hence increased by up to 0.8 % absolute.

Documents:

02324-kolnp-2007-abstract.pdf

02324-kolnp-2007-assignment.pdf

02324-kolnp-2007-claims.pdf

02324-kolnp-2007-correspondence others-1.1.pdf

02324-kolnp-2007-correspondence others.pdf

02324-kolnp-2007-description complete.pdf

02324-kolnp-2007-drawings.pdf

02324-kolnp-2007-form 1.pdf

02324-kolnp-2007-form 3-1.1.pdf

02324-kolnp-2007-form 3.pdf

02324-kolnp-2007-form 5.pdf

02324-kolnp-2007-international publication.pdf

02324-kolnp-2007-international search report.pdf

02324-kolnp-2007-pct request form.pdf

02324-kolnp-2007-priority document.pdf

2324-KOLNP-2007-(02-07-2014)-ABSTRACT.pdf

2324-KOLNP-2007-(02-07-2014)-ANNEXURE TO FORM 3.pdf

2324-KOLNP-2007-(02-07-2014)-CLAIMS.pdf

2324-KOLNP-2007-(02-07-2014)-CORRESPONDENCE.pdf

2324-KOLNP-2007-(02-07-2014)-DESCRIPTION (COMPLETE).pdf

2324-KOLNP-2007-(02-07-2014)-DRAWINGS.pdf

2324-KOLNP-2007-(02-07-2014)-FORM-1.pdf

2324-KOLNP-2007-(02-07-2014)-FORM-13.pdf

2324-KOLNP-2007-(02-07-2014)-FORM-2.pdf

2324-KOLNP-2007-(02-07-2014)-OTHERS.pdf

2324-KOLNP-2007-(02-07-2014)-PETITION UNDER RULE 137.pdf

2324-KOLNP-2007-(22-07-2014)-CORRESPONDENCE.pdf

2324-KOLNP-2007-(22-07-2014)-OTHERS.pdf

2324-KOLNP-2007-CORRESPONDENCE.pdf

2324-kolnp-2007-form-18.pdf

2324-KOLNP-2007-PA.pdf


Patent Number 265925
Indian Patent Application Number 2324/KOLNP/2007
PG Journal Number 13/2015
Publication Date 27-Mar-2015
Grant Date 24-Mar-2015
Date of Filing 22-Jun-2007
Name of Patentee FORSCHUNGSZENTRUM JÜLICH GMBH
Applicant Address WILHELM-JOHNEN-STRASSE 52425 JÜLICH
Inventors:
# Inventor's Name Inventor's Address
1 CARIUS, REINHARD KOMMSTRASSE 8, 52428, JÜLICH GERMANY
2 KLEIN STEFAN BERGWERKSTRASSE1A, 63796 KAHLAM MAIN
3 FINGER, FRIEDHELM AM SCHÜTZENHOF 4, 52428, JÜLICH GERMANY
4 MAI, YAOHUA WIESENSTR. 8, 52428, JÜLICH GERMANY
PCT International Classification Number H01L 31/18
PCT International Application Number PCT/DE2005/002237
PCT International Filing date 2005-12-13
PCT Conventions:
# PCT Application Number Date of Convention Priority Country
1 102004 061360.5 2004-12-21 Germany